The common failure modes of bitumen joint and crack sealants, from adhesion loss to tracking and stone intrusion, and what causes each one.

Written by the Nuroil trade desk, Sharjah

NURMASTIC rubberized bitumen sealant
On this page · 6 sections
  1. 01Adhesion failure
  2. 02Cohesive failure
  3. 03Softening, tracking and pull-out
  4. 04Stone intrusion and spalling
  5. 05Ageing and hardening
  6. 06What to ask for when buying

A well-placed bitumen sealant should keep water and incompressible grit out of a pavement joint for several years. When seals fail early, the cause is rarely the product alone. Most failures trace back to joint preparation, the wrong sealant type for the climate, poor heating practice or a joint shape that overstresses the material. Knowing the failure modes helps buyers and contractors choose the right product and specify the work properly.

Adhesion failure

Adhesion failure is the most common problem: the sealant pulls cleanly away from one or both joint walls, leaving a thin gap that lets water straight in. It usually starts in the coldest weather when the joint is at its widest and the sealant is at its stiffest.

  • Causes: dust, laitance or old sealant left on the joint walls; moisture in the joint at the time of sealing; pouring sealant that has cooled too far to wet the surface; sealant bonded to the bottom of the joint as well as the sides (three-sided adhesion).
  • Prevention: clean both faces thoroughly, blow out with dry, oil-free compressed air, seal only when surfaces are dry and the weather is suitable, and use a heat-resistant backer rod or bond breaker in concrete joints so the sealant bonds only to the walls.

Cohesive failure

In cohesive failure the sealant splits through its own body while staying stuck to the walls. It means the material could not stretch as far as the joint moved.

  • Causes: a sealant type with insufficient low-temperature extension for the climate; a sealant bead that is too deep relative to its width; sealant degraded by overheating or prolonged heating in the melter.
  • Prevention: match the specification type or class to the climate (for example ASTM D6690 Type IV is tested at higher extension for very cold regions), follow the recommended width-to-depth ratio, and keep melter temperatures within the producer's limits.

Softening, tracking and pull-out

In hot weather a sealant that is too soft can flow out of the joint, stick to tyres and be pulled out in strings, leaving the joint empty and the road surface marked. Overbanding a wide film of sealant on the road surface makes this worse because the exposed material is heated by the sun and contacted by tyres.

  • Causes: a softening point or flow resistance too low for local pavement temperatures; overfilling or wide overbands; opening to traffic before the sealant has cooled.
  • Prevention: specify a product with adequate softening point and flow resistance for hot climates, keep overbands narrow and thin, and keep traffic off until the sealant is tack-free.

Stone intrusion and spalling

If a joint is underfilled or the sealant has lost adhesion, small stones and grit get into the gap. When the slab expands in summer, these incompressibles concentrate stress at the joint edges and can spall the concrete. Keeping joints fully sealed is the main defence; regular inspection lets crews reseal before damage spreads.

Ageing and hardening

Like all bitumen products, sealants oxidise and harden over time under sun and heat, which gradually reduces their ability to stretch. EN 13880 includes a heat stability test that compares cone penetration before and after prolonged heating to show how much a compound stiffens. Products with higher elastic recovery generally tolerate ageing better, but every seal eventually needs replacing.

SymptomLikely causeCheck
Clean gap between sealant and joint wallDirty or damp joint, cold pour, three-sided bondCleaning method, weather records, backer rod
Split through the middle of the beadWrong type for climate, bead too deep, overheated materialSpecified type, joint shape, melter log
Sealant on tyres and road surfaceToo soft for climate, overband too wide, early traffickingSoftening point, overband width
Chipped joint edgesIncompressibles in open jointFill level and inspection interval

What to ask for when buying

Most failures can be avoided at the specification stage. In your enquiry, state the pavement type, climate range, joint dimensions and expected movement, and the standard and type required. Ask the supplier for the technical data sheet, including recommended pouring temperature, maximum safe heating temperature and maximum heating time, plus the SDS and a batch certificate of analysis showing cone penetration, resilience and softening point. Nuroil provides a CoA with every delivery of bitumen sealant, and third-party inspection can be arranged on request.

PRODUCTS IN THIS ARTICLE
KEEP READING

More from the Knowledge Centre.

STILL HAVE A QUESTION?

Ask the people who trade it every day.