A common site complaint goes like this: a steel gate, gutter or masonry plinth was coated with black bitumen paint, and later someone wants it painted grey, white or green. Within days the new paint shows brown stains, stays tacky or wrinkles. The cause is bleed-through, and it is well known to coating suppliers. Several bitumen paint data sheets warn directly that the product may bleed through any paint applied over it.
What bleed-through is
Bitumen is soluble in many of the hydrocarbon solvents used in conventional paints. When a solvent-borne topcoat is applied, its solvent partly redissolves the bitumen beneath. Dark, oily bitumen fractions then migrate into the new film, staining it brown or black and sometimes preventing it from hardening properly. Paint inspection guides describe bleeding as a partial or full redissolving of the previous coat, and note that strong solvents in the topcoat make it worse.
Signs to look for
- Brown or yellow discolouration appearing through a light-coloured topcoat.
- Patches that stay soft or sticky long after the rest has dried.
- Wrinkling or lifting where the topcoat solvent has attacked the bitumen layer.
- Staining that returns after a further coat of the same topcoat.
How to avoid it
The simplest answer is to decide at the start whether the surface will ever need a decorative finish. If it will, bitumen paint may not be the right first coat. Where bitumen paint is already in place, options include:
- Use an isolating sealer. Data sheets advise applying a primer recommended by the topcoat manufacturer before overpainting. Aluminium-pigmented sealers are a traditional choice for isolating bitumen and tar, because the flake pigment forms a barrier layer.
- Allow full drying first. Bitumen paint that is still releasing solvent is more easily disturbed.
- Test a small area. Apply the sealer and topcoat to a patch and wait several days before judging.
- Remove it if the problem is severe. Refinishing guides advise isolating the whole area or, where bleeding is heavy, removing coatings back to a sound substrate and starting again with a correct primer and topcoat.
Why water-based topcoats are not a guaranteed fix
It is tempting to assume that a water-based topcoat will avoid the problem because it contains little or no hydrocarbon solvent. It usually reduces the risk of the bitumen redissolving, but adhesion is another matter. Bitumen films are soft and slightly oily, and many water-based paints do not wet or grip them well, so they can peel or crack as the bitumen moves with temperature. A trial patch remains essential whatever topcoat is chosen.
Bitumen over other coatings
The reverse problem also exists. Applying solvent-borne bitumen paint over a fresh or soft coating can lift or wrinkle it. Check that any existing coating is fully cured and compatible, and test first.
Bitumen paint over bitumen paint
Recoating black bitumen paint with more of the same is normally straightforward. Clean off dirt and loose material, allow the previous coat to dry as the data sheet requires, and apply the next coat. Recoat intervals on published data sheets range from a few hours to about a day.
| Situation | Risk | Usual approach |
|---|---|---|
| Bitumen paint over bitumen paint | Low | Clean, recoat after drying |
| Solvent-borne paint over bitumen paint | High | Isolating sealer, trial patch |
| Bitumen paint over cured coating | Moderate | Check compatibility, trial patch |
| Decorative finish required later | High | Choose a different system from the start |
If a surface may one day need colour, plan for it before the first coat of bitumen goes on.
Specifying to avoid the problem
When ordering, tell the supplier whether the bitumen-painted surface will be overcoated and with what. Ask for the TDS, which should state overpainting limitations, and the SDS for the solvent type. More on the product Nuroil supplies is on the bitumen paint page, and you can raise questions through contact us.