Plants that burn furnace oil sometimes find perforated economiser tubes, corroded air preheater elements or a stack liner eaten away near the top. The cause is usually the same: sulphuric acid condensing on metal that runs too cold. This is known as cold-end or acid dew point corrosion, and it links directly to the sulphur content of the fuel.
How the acid forms
Furnace oil contains sulphur, and specifications allow several percent by mass in the heavier grades. In the flame, almost all of it burns to sulphur dioxide. A small share is oxidised further to sulphur trioxide. In the cooler parts of the boiler, sulphur trioxide combines with water vapour from combustion to form sulphuric acid vapour.
As long as the gas and the surfaces it touches stay above the acid dew point, the acid remains a vapour and passes up the stack. Where any metal surface sits below that dew point, acid condenses as a film and attacks carbon steel. Because the dew point of sulphuric acid is far higher than that of plain water, a surface can be dry by ordinary standards and still collect acid.
Where the damage appears
- Economisers. The tube wall runs close to the feedwater temperature, not the flue gas temperature, because heat transfer on the water side is much better. Cold feedwater therefore means a cold tube wall, even when the gas is hot.
- Air preheaters. The cold end, where incoming air meets outgoing gas, is the most exposed point.
- Ducts, dampers and stacks. Poorly insulated sections, areas with air in-leakage and stack tops cool the gas locally.
- During start-up and low load. Surfaces are cold and gas temperatures are low, so acid condenses even on units that are fine at full load.
Why oil firing is more sensitive
Indicative figures published for boiler designers put the acid dew point for heavy fuel oil well above that for light fuel oil, and both far above natural gas, where the ordinary water dew point governs. Ash from residual oil also contains vanadium, which can encourage more sulphur trioxide to form and makes deposits more aggressive. Deposits on cold surfaces absorb acid and hold it against the metal, so fouling and corrosion tend to feed each other.
The acid dew point, not the fuel saving you want, sets the lowest safe metal temperature at the cold end of a conventional oil-fired boiler.
Ways to limit cold-end corrosion
- Keep metal temperatures up. Raise feedwater temperature entering the economiser, or bypass part of the air preheater during low-load operation. Do not chase extra efficiency by lowering exit gas temperature below the designer's limit for the fuel.
- Control excess air. Running with more air than needed raises the share of sulphur that ends up as sulphur trioxide. Good burner tuning with stable, low excess air helps.
- Choose fuel sulphur deliberately. A lower-sulphur grade lowers the dew point. If the plant has a history of cold-end damage, the cost difference may be worth it.
- Consider fireside additives. Magnesium-based additives have been used on oil-fired units to neutralise acid and reduce deposits. Use them under the guidance of the boiler maker or a specialist.
- Wash carefully. Water washing of oil-fired surfaces can leave acidic salts behind if the final rinse is not neutralised, typically with a mild alkaline solution. Dry the unit promptly after washing.
- Inspect and measure. Visual checks at shutdowns and ultrasonic wall-thickness readings on economiser tubes show where corrosion is advancing.
Fuel quality factors to watch
Sulphur content has the biggest effect on the acid dew point. Vanadium and sodium in the ash influence deposit chemistry and high-temperature corrosion. Water and sediment matter for burner performance, which in turn affects how much excess air the plant needs to run cleanly. Asking for these values on every certificate of analysis helps link any change in boiler condition to a change in fuel.
Specifying fuel with corrosion in mind
When you enquire for furnace oil, give the maximum sulphur content your boiler and emission permit allow and ask for sulphur, ash and, where relevant, vanadium on the certificate of analysis. If you are deciding between grades, the furnace oil page lists what Nuroil can supply, and our team can quote alternatives through the quote form.